Height Adjustable Stand

Let’s look at the back side of the socket weld to see what kind of penetration I got:

7177D2EB-657A-4A33-B801-FD5FC17EB175.png

I am not so impressed with this penetration.
 
Here is the .082” or so tubing (main mast/outside tube) on the 1/2” plate.

3 autogenous tack welds, 1 regular tack weld, 360° around autogenous (skipping around), lay wire technique with 3/32” filler rod (not skipping around), & the weld did not need washing.

150A max & usually using all of it.

42AB17BF-3933-49C4-AA49-A9BE67D1B6AE.png

CF488120-BB08-434C-9DEE-8D42A89DFADE.png

F42677C7-C83F-436F-95CA-AAB3DEDCB653.png

DEA26448-0C8F-485A-8595-88CE37DC9940.png

See undercut in tubing, third picture down. Can you say stress riser?
 
Back